Delta Fastener Corp. can provide a wide variety of fasteners, nuts, bolts, sockets, washers and more in MP35N. If we do not have your item in stock (Inch or Metric) we can have these manufactured to your specification.
Carpenter MP35N alloy is a nonmagnetic, nickel-cobalt-chromium-molybdenum alloy possessing a unique combination of ultrahigh tensile strength (up to 300 ksi [2068 MPa]), good ductility and toughness, and excellent corrosion resistance. In addition, this alloy displays exceptional resistance to sulfidation, high temperature oxidation, and hydrogen embrittlement. The unique properties of MP35N alloy are developed through work hardening, phase transformation and aging. If the alloy is used in the fully work hardened condition, service temperatures up to 750°F (399°C) are suggested. MP35N alloy is normally produced by vacuum induction melting (VIM), followed vacuum arc remelting (VAR).
Because of its unique combination of properties, MP35N alloy has been used in a wide variety of applications. MP35N alloy has been used in fasteners, springs, nonmagnetic electrical components and instrument parts in medical, seawater, oil and gas well, and chemical and food processing environments. *MP35N is a trademark of SPS Technologies, Inc. MP is a registered trademark of SPS Technologies, Inc.
Physical Properties | Metric | English | Comments |
Density | 8.43 g/cc | 0.305 lb/in3 |
Mechanical Properties | Metric | English | Comments |
Tensile Strength, Ultimate | 931 MPa | 135000 psi | |
Tensile Strength, Yield | 414 MPa @Strain 0.200 % | 60000 psi @Strain 0.200 % | |
Elongation at Break | 70.0 % | 70.0 % | |
Reduction of Area | 70.0 % | 70.0 % | |
Modulus of Elasticity | 232.8 GPa | 33770 ksi | |
Shear Modulus | 83.36 GPa | 12090 ksi |
Electrical Properties | Metric | English | Comments |
Electrical Resistivity | 0.0001033 ohm-cm | 0.0001033 ohm-cm | Room Temp. 1.154E-4 Ohm-cm at 538°C |
Thermal Properties | Metric | English | Comments |
CTE, linear | 12.8 µm/m-°C @Temperature 21.0 - 93.0 °C | 7.11 µin/in-°F @Temperature 69.8 - 199 °F | |
14.8 µm/m-°C @Temperature 21.0 - 316 °C | 8.22 µin/in-°F @Temperature 69.8 - 601 °F | ||
15.7 µm/m-°C @Temperature 21.0 - 538 °C | 8.72 µin/in-°F @Temperature 69.8 - 1000 °F | ||
Thermal Conductivity | 11.2 W/m-K | 77.7 BTU-in/hr-ft2-°F | at room Temp. 17.0 W/m-K at 316°C. 23.4 W/m-K at 649°C. |
Melting Point | 1315 - 1440 °C | 2399 - 2620 °F | |
Solidus | 1315 °C | 2399 °F | |
Liquidus | 1440 °C | 2620 °F |
Component Elements Properties | Metric | English | Comments |
Boron, B | 0.010 % | 0.010 % | |
Carbon, C | <= 0.025 % | <= 0.025 % | |
Chromium, Cr | 19.0 - 21.0 % | 19.0 - 21.0 % | |
Cobalt, Co | 33.0 % | 33.0 % | as remainder |
Iron, Fe | <= 1.0 % | <= 1.0 % | |
Manganese, Mn | <= 0.15 % | <= 0.15 % | |
Molybdenum, Mo | 9.0 - 10.5 % | 9.0 - 10.5 % | |
Nickel, Ni | 33.0 - 37.0 % | 33.0 - 37.0 % | |
Phosphorous, P | <= 0.015 % | <= 0.015 % | |
Silicon, Si | <= 0.15 % | <= 0.15 % | |
Sulfur, S | <= 0.010 % | <= 0.010 % | |
Titanium, Ti | <= 1.0 % | <= 1.0 % |
Data provided by Carpenter Technology Corporation.
Disclaimer: The dimensions listed are for reference only. Sizes not listed may be available off the shelf or can be manufactured to customer requirements.